A dent, a cut or a patch of corrosion found at a visual inspection doesn’t retire a cylinder by itself, but every kind of defect has a limit. Most limits depend on the outside diameter or the minimum design wall thickness, so the same 0.5 mm pit can pass on one cylinder and fail on another.
Pick the standard (ISO-18119, or CGA C-6 and C-6.1 for US steel and aluminium cylinders), pick the defect and enter what you measured. The calculator shows pass or fail for each rule, the limit, and how much margin is left or by how much the defect is over.
Background
What it checks
Pick the rules the cylinder is inspected to and the defect you found, then enter what you measured. Each rule shows pass or fail, its limit, and how much room is left or how far the defect is over. When several rules apply, the one closest to failing, or furthest over, is the binding rule. A value exactly on a limit passes, except where the standard says ‘less than’.
The minimum design wall thickness and the wall next to the defect are optional. Leave them empty if you don’t have them: the checks that need them are skipped, and the result says which.
ISO-18119 covers seamless steel and aluminium cylinders in Europe and most of the world. CGA C-6 (steel, DOT-3A and DOT-3AA) and CGA C-6.1 (aluminium, DOT-3AL) are the US rules; the C-6 rules here are those for high-pressure cylinders, 900 psi service pressure and up.
Depth limits
Most limits are a share of the minimum design wall thickness, not of the wall you measure:
d \le k \cdot t_\text{min}dDepth of the defect in mmkAllowed share, from the table belowt_\text{min}Minimum design wall thickness in mm| Defect | ISO-18119 | CGA C-6.1 |
|---|---|---|
| Cut or gouge | 10 % | 10 % |
| General corrosion | 10 % | 10 % |
| Local corrosion | 20 % | – |
| Line corrosion | 10 % | 10 % |
| Isolated pit | – | 30 % |
| Crevice corrosion | 20 % | – |
ISO-18119 calls corrosion that covers more than 20 % of the inside or outside surface general, and less than 20 % local; exactly 20 % is taken as general here. A pit 5 mm or more across counts as local corrosion. A cut only counts as one when it is deeper than 5 % of t_\text{min}.
Under ISO-18119, line corrosion is rejected when it is longer than the outside diameter and deeper than 10 % of t_\text{min}.
Without t_\text{min}, CGA C-6.1 uses fixed depths: 1/32 in (0.79 mm) for cuts, general and line corrosion, 1/16 in (1.59 mm) for pits. C-6.1 states its corrosion limits for walls of 3/16 in (4.76 mm) and more. ISO-18119 and CGA C-6 have no such fallback: without the design wall their wall-based checks are skipped.
Remaining wall
t_r = t_s - dt_rRemaining wall at the deepest point in mmt_sWall next to the defect (ultrasonic reading) in mmdDepth of the defect in mmISO-18119: t_r must be at least t_\text{min} for cuts and every type of corrosion. CGA C-6 works with the remaining wall alone, against an in-service limit:
t_\text{is} = 0.95 \cdot t_dt_\text{is}In-service limiting wall thickness in mmt_dMinimum allowable design thickness in mmIf the wall next to the defect wasn’t measured, C-6 takes t_d - d as the remaining wall, so the depth may be at most 5 % of t_d. Isolated pits may go to a third of t_d, as long as they are narrower than 2 \cdot t_d and 0.6 in (15 mm) and the next pit’s centre is further away than both diameters added; a wider pit is judged as general corrosion. Without t_d, C-6 condemns general corrosion over more than 20 % of the surface.
For DOT-3A and DOT-3AA cylinders, C-6 Table 3 gives t_d from the outside diameter:
t_d = f \cdot Dt_dMinimum allowable design thickness in mmfFactor for the DOT marking, C-6 Table 3DOutside diameter in mmThe table’s in-service column gives t_\text{is} the same way; it is 95 % of the first, rounded.
Dents
ISO-18119 counts a depression as a dent when it is deeper than 1 % of the outside diameter. It may be at most:
d \le 0.03 \cdot DdDepth of the dent in mmDOutside diameter in mmand it must be wide enough:
w \ge 15 \cdot dwDiameter of the dent in mmdDepth of the dent in mmCGA C-6 and C-6.1: a dent may be up to 1/16 in (1.59 mm) deep if its largest diameter is at least 2 in (50.8 mm); smaller dents are condemned at any depth. C-6 gives this as industry practice, stated for a cylinder of 9 in by 51 in.
Lengths, areas, threads and weight
- ISO-18119: a cut may be at most 25 % of the outside diameter long.
- CGA C-6.1: cuts and line corrosion must stay shorter than 3 in (76.2 mm). General corrosion may cover at most 3 in² (19.4 cm²), inside and outside added; where it sits at the same spot inside and outside, add the two depths.
- Threads: ISO-18119 leaves the number of full threads to the cylinder maker. CGA C-6 asks for at least 7 continuous full threads on a tapered neck and 6 on a straight one.
- CGA C-6: a cylinder that weighs less than 95 % of its stamped tare weight is rejected (not for cylinders of more than 500 lb, 227 kg, water capacity).
How to measure
- Clean the defect back to bare metal first. Depth can’t be judged through rust.
- Outside diameter: measure round the cylinder with a tape or a piece of string and divide by π.
- Dent depth: a straight edge and calliper, or a pipe pit gauge. Width: ISO-18119 asks for the diameter of the dent, take the smallest width you find; CGA uses the largest (major) diameter.
- Cuts and pits: a pit gauge or depth gauge. Smooth off raised metal at the edges first.
- Wall next to the defect: an ultrasonic thickness gauge on sound metal right beside it. Most single-echo gauges count the paint as metal: measure on bare metal or subtract the coating.
- Inside corrosion: the ultrasonic reading on sound metal minus the reading at the deepest point gives the depth.
- Tare weight: weigh the cylinder the way the stamped value was taken, with or without valve.
- Corroded share: compare the corroded area with the surface of the cylindrical part.
A = \pi \cdot D \cdot LASurface of the cylindrical part in cm²DOutside diameter in cmLLength of the cylindrical part in cmReject on sight
Nothing to calculate for these: cracks, including neck cracks; bulges; fire or heat damage (melted or distorted metal; charred paint needs a hardness test; CGA C-6.1 condemns aluminium heated to 177 °C, 350 °F); arc or torch burns; lamination (ISO-18119: inside always, outside unless it can be ground out with the wall still at t_\text{min}); extra holes, plugs or inserts; altered or illegible stamping; suspicious marks that can’t be cleared up; a cylinder that won’t stand upright; folds reaching more than two full threads (CGA C-6.1); and corrosion where the original surface can’t be made out after cleaning.
This is a workbench aid. The full standard and the cylinder maker’s criteria govern.